Heat Distortion Temperature of 30% Glass Fiber Reinforced Polymers at 1.82 MPa

Polymer (30% GF) HDT (°C)
Acrylonitrile-butadiene-styrene (ABS) 99
Polystyrene (PS) 122
Polyphenylene ether (PPE, PPO) 139
Polypropylene (PP) 142
Polycarbonate (PC) 142
Polyacetal (POM) 159
Polycaprolactam (PA6, Nylon 6) 207
Polybutylene terephthalate (PBT) 209
Polyetherimides (PEI) 209
Polyether sulfone (PES, PSU) 211
Polyphenylsulfone (PPSU) 215
Polyethylene terephthalate (PET) 219
Polyphthalamides (PPA) 243
Polyhexamethylene adipamide (PA66, Nylon 6,6) 253
Polyphenylene sulfide (PPS) 268
Polyamideimide (PAI) 281
Polyetheretherketone (PEEK) 315
Polyetherketone (PEK) 319
(1) The heat deflection temperatures (HDT) are the average of one or more experimental values.