Heat Distortion Temperature of Neat Polymers at 1.82 MPa / 264 psi
Polymer |
HDT (°C) |
High Density Polyethylene (HDPE) |
46 |
Polybutylene terephthalate (PBT) |
56 |
Polypropylene (PP) |
62 |
Polycaprolactam (PA6, Nylon 6) |
64 |
Polyethylene terephthalate (PET) |
71 |
Polyhexamethylene adipamide (PA66, Nylon 6,6) |
74 |
Polystyrene (PS) |
79 |
Polymethyl methacrylate (PMMA) |
83 |
Acrylonitrile-butadiene-styrene (ABS) |
94 |
Polyacetal (POM) |
106 |
Polyphenylene ether (PPE, PPO) |
114 |
Polyphenylene sulfide (PPS) |
120 |
Polycarbonate (PC) |
124 |
Polyphthalamides (PPA) |
127 |
Polyetheretherketone (PEEK) |
159 |
Polyetherketone (PEK) |
169 |
Polyetherimides (PEI) |
199 |
Polyether sulfone (PES, PSU) |
206 |
Polyphenylsulfone (PPSU) |
206 |
Polyamideimide (PAI) |
278 |
Polyimide (PI) |
319 |
Polybenzimidazole (PBI) |
425 |
|
|