Required Temperature (°C) For One Hour And Ten Hours Half-life

Initiator T(°C) - 1 h T(°C) - 10 h
Ammoniumperoxodisulfate 87 69
1,1’-Azodi(hexahydrobenzonitrile) 103 85
2,2’-Azodi(2-methylbutyronitrile)  84 66
2,2’-Azodi(isobutyronitrile)  81 63
Butyl 4,4-di(tert-butylperoxy)valerate 125 102
Cumyl hydroperoxide 166 140
Cumyl peroxyneodecanoate 55 38
Cumyl peroxyneoheptanoate  59 42
Di(2-ethylhexyl) peroxydicarbonate 64 47
Di(3,5,5-trimethylhexanoyl) peroxide  78 59
Di(3-methoxybutyl) peroxydicarbonate  57 43
2,3-Dimethyl-2,3-diphenylbutane 247 224
2,5-Dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane 85 68
2,5-Dimethyl-2,5-di(tert-butylperoxy)hexane 139 118
2,5-Dimethyl-2,5-di(tert-butylperoxy)hexyne-3 147 124
Di(4-methylbenzoyl)peroxide 89 70
Di-(tert-amyl)-peroxide 135 113
Di(tert-butyl)peroxide  144 123
2,2-Di(tert-butylperoxy)butane 120 101
Di(4-tert-butylcyclohexyl) peroxydicarbonate 64 48
1,1-Di(tert-amylperoxy)cyclohexane 106 87
1,1-Di(tert-butylperoxy)-3,5,5-trimethylcyclohexane 110 90
1,1-Di(tert-butylperoxy)cyclohexane 115 96
Di(tert-butylperoxy-isopropyl)benzene  138 117
Dibenzoyl peroxide 91 72
Dicetyl peroxydicarbonate  65 48
Dicumyl peroxide 135 114
Didecanoyl peroxide  80 63
Diisobutyryl peroxide 39 23
Diisopropyl peroxydicarbonate  64 47
Dilauroyl peroxide 79 61
Dimyristyl peroxydicarbonate 65 48
Di-sec-butyl peroxydicarbonate  63 47
Isopropylcumyl hydroperoxide  154 129
Isopropylcumyl hydroperoxide  154 129
tert-Amyl hydroperoxide 190 153
tert-Amyl peroxy-2-ethylhexanoate 91 73
tert-Amyl peroxyacetate 114 96
tert-Amyl peroxy-benzoate 120 101
tert-Amyl peroxyneodecanoate 62 44
tert-Amyl peroxypivalate 72 54
tert-Amylperoxy-(2-ethylhexyl)carbonate 113 95
tert-Butyl cumyl peroxide 137 117
tert-Butyl hydroperoxide 193 169
tert-Butyl peroxy-2-ethylhexanoate 92 73
tert-Butyl peroxy-3,5,5-trimethyl-hexanoate 117 97
tert-Butyl peroxydiethylacetate 93 75
tert-Butyl peroxy-isobutyrate 97 78
tert-Butyl peroxyneodecanoate 64 47
tert-Butyl peroxyneoheptanoate 68 50
tert-Butyl peroxypivalate 75 57
tert-Butyl-monoperoxy-maleate 104 82
tert-Butylperoxy isopropyl carbonate 117 98
tert-Butylperoxy-(2-ethylhexyl)carbonate  120 99
tert-Butylperoxy-acetate  120 101
tert-Butylperoxybenzoate  124 104
1,1,3,3-Tetramethylbutyl hydroperoxide 159 140
1,1,3,3-Tetramethylbutyl peroxy-2-ethylhexanoate 88 69
1,1,3,3-Tetramethylbutyl peroxyneodecanoate 57 40
1,1,3,3-Tetramethylbutyl peroxypivalate 66 48
3,6,9-Triethyl-3,6,9-trimethyl-1,4,7-triperoxonane 146 125

Initiator