Q and e Experimental valuesa
Vinyl
Monomer |
e |
Q |
Maleic anhydride |
2.97 |
0.55 |
Diethyl Fumarate |
2.26 |
0.24 |
Acrylic Acid |
1.11 |
0.76 |
Acrylonitrile |
0.91 |
0.40 |
Vinyl methyl ketone |
0.87 |
0.68 |
Hydroxypropyl acrylate |
0.75 |
0.92 |
n-Butyl acrylate |
0.74 |
0.32 |
Methacrylonitrile |
0.69 |
0.86 |
Methacrylic acid |
0.64 |
1.66 |
Methyl acrylate |
0.50 |
0.31 |
Hydroxyethyl methacrylate |
0.30 |
0.87 |
Methyl methacylate |
0.30 |
0.57 |
Vinylidene chloride |
0.24 |
0.20 |
t-Butyl methacrylate |
0.24 |
0.74 |
Vinyl chloride |
0.07 |
0.13 |
Vinyl acetate |
-0.28 |
0.02 |
1,3 Butadiene |
-0.59 |
1.66 |
Styrene |
-0.80 |
1.00 |
α-Methylstyrene |
-1.04 |
0.98 |
Ethyl vinyl ether |
-1.49 |
0.03 |
t-Butyl vinyl ether |
-1.58 |
0.15 |