Activation Energy For the Initiator Dissociation

Initiator Ea (kJ/mol)
Ammoniumperoxodisulfate 135.0
1,1’-Azodi(hexahydrobenzonitrile) 142.2
2,2’-Azodi(2-methylbutyronitrile)  128.9
2,2’-Azodi(isobutyronitrile)  130.1
Butyl 4,4-di(tert-butylperoxy)valerate 143.5
Cumyl hydroperoxide 132.6
Cumyl peroxyneodecanoate 114.8
Cumyl peroxyneoheptanoate  114.3
Di(2-ethylhexyl) peroxydicarbonate 122.5
Di(3,5,5-trimethylhexanoyl) peroxide  122.7
Di(3-methoxybutyl) peroxydicarbonate  143.3
2,3-Dimethyl-2,3-diphenylbutane 212.6
2,5-Dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane 133.9
2,5-Dimethyl-2,5-di(tert-butylperoxy)hexane 148.7
2,5-Dimethyl-2,5-di(tert-butylperoxy)hexyne-3 152.3
Di(4-methylbenzoyl)peroxide 125.0
Di-(tert-amyl)-peroxide 138.7
Di(tert-butyl)peroxide  152.7
2,2-Di(tert-butylperoxy)butane 148.5
Di(4-tert-butylcyclohexyl) peroxydicarbonate 126.4
1,1-Di(tert-amylperoxy)cyclohexane 139.5
1,1-Di(tert-butylperoxy)-3,5,5-trimethylcyclohexane 135.3
1,1-Di(tert-butylperoxy)cyclohexane 140.2
Di(tert-butylperoxy-isopropyl)benzene  147.3
Dibenzoyl peroxide 124.2
Dicetyl peroxydicarbonate  124.3
Dicumyl peroxide 152.3
Didecanoyl peroxide  128.2
Diisobutyryl peroxide 109.1
Diisopropyl peroxydicarbonate  124.0
Dilauroyl peroxide 123.4
Dimyristyl peroxydicarbonate 124.1
Di-sec-butyl peroxydicarbonate  123.9
Isopropylcumyl hydroperoxide  131.4
Isopropylcumyl hydroperoxide  131.4
tert-Amyl peroxy-2-ethylhexanoate 129.1
tert-Amyl peroxyacetate 152.2
tert-Amyl peroxy-benzoate 145.0
tert-Amyl peroxyneodecanoate 113.7
tert-Amyl peroxypivalate 124.4
tert-Amylperoxy-(2-ethylhexyl)carbonate 149.7
tert-Butyl cumyl peroxide 150.5
tert-Butyl hydroperoxide 167.5
tert-Butyl peroxy-2-ethylhexanoate 130.0
tert-Butyl peroxy-3,5,5-trimethyl-hexanoate 143.9
tert-Butyl peroxydiethylacetate 134.0
tert-Butyl peroxy-isobutyrate 132.6
tert-Butyl peroxyneodecanoate 118.2
tert-Butyl peroxyneoheptanoate 116.8
tert-Butyl peroxypivalate 116.8
tert-Butyl-monoperoxy-maleate 116.0
tert-Butylperoxy isopropyl carbonate 150.2
tert-Butylperoxy-(2-ethylhexyl)carbonate  139.9
tert-Butylperoxy-acetate  149.2
tert-Butylperoxybenzoate  147.3
1,1,3,3-Tetramethylbutyl hydroperoxide 182.0
1,1,3,3-Tetramethylbutyl peroxy-2-ethylhexanoate 123.8
1,1,3,3-Tetramethylbutyl peroxyneodecanoate 116.4
1,1,3,3-Tetramethylbutyl peroxypivalate 117.5
3,6,9-Triethyl-3,6,9-trimethyl-1,4,7-triperoxonane 150.2
   

Activation
Energy

Numerical List