Van der Waals Volume of Repeating Units
Polymer |
VVdW1
(cm3/mol) |
Poly(vinyl chloride), PVC | 29.5 |
Poly(vinyl fluoride), PVF | 23.7 |
Poly(vinylidene fluoride), PVDF | 26.9 |
Polychloroprene, Neoprene | 46.9 |
Poly(tetrafluoroethylene) | 33.1 |
Poly(acrylic acid), PAA | 36.3 |
Poly(ethyl acrylate) , PEA | 58.2 |
Poly(methyl acrylate), PMA | 47.9 |
Poly(cyclohexyl acrylate) | 92.1 |
Poly(1-butene), PB-1 | 41.1 |
Poly(ethylene), PE | 20.6 |
Poly(isobutene) | 41.1 |
Poly(propylene), PP | 30.8 |
Poly(8-aminooctanoic acid), Nylon 8 | 90.3 |
Poly(caprolactam), Nylon 6 | 69.9 |
Poly(hexamethylene adipamide), Nylon6,6 | 139.6 |
Poly(hexamethylene dodecanediamide), Nylon 6,12 | 201.1 |
Poly(m-phenylene terephthalamide), Nomex MPDI | 126.0 |
Poly(p-phenylene terephthalamide) (spun), Kevlar, PPTA | 126.0 |
Poly(ω-dodecanamide), Nylon 12 | 131.3 |
Poly(ω-undecanamide), Nylon 11 | 121.0 |
Poly(Bisphenol A carbonate), PC | 143.8 |
Poly(butyl cyanoacrylate) | 90.3 |
PoIy(1,2-butadiene) | 38.7 |
Poly(1,4-butadiene), PBD | 38.7 |
Poly(ethylene terephthalate), PET | 100.0 |
Poly[(ether ether ketone) PEEK | 157.8 |
Poly(ethylene glycol), PEO, PEG | 26.4 |
Poly(propylene glycol), PPG | 36.4 |
Poly(tetrahydrofuran), PTMO, PTHF | 46.9 |
Polyacetal, Poly(methylene oxide), POM | 16.4 |
Poly(butyl methacrylate), PBMA | 88.9 |
Poly(cyclohexyl methacrylate), PCHMA | 109.6 |
Poly(ethyl methacrylate), PEMA | 68.4 |
Poly(methyl methacrylate), PMMA | 58.1 |
Poly(acrylonitrile), PAN | 32.5 |
Poly(methacrylonitrile) | 42.8 |
Poly(acrylamide) | 38.7 |
Poly(2-methylstyrene) | 75.9 |
Poly(4-methylstyrene), PMS, PPMS | 75.9 |
Poly(4-tert-butylstyrene) | 107.3 |
Poly(α-methylstyrene), PAMS | 76.5 |
Polystyrene, PS | 66.1 |
Poly(1,4-biphenyl ether ether sulfone), PPSU | 202.0 |
Poly(1,4-phenylene ether-sulfone), PES | 108.9 |
Poly{[bis(4-chlorophenyl)sulfone]-alt-[bisphenol-A]}, PSU | 232.8 |
Poly(thio-1,4-phenylene), PPS | 56.8 |
Poly(vinyl alcohol), PVOH | 25.0 |
Poly(vinyl acetate), PVA, PVAC | 47.9 |
Poly(butyl vinyl ether) | 67.4 |
Poly(ethyl vinyl ether) | 46.6 |
Poly(methyl vinyl ether), PVME | 36.6 |