Polymer-Solvent Interaction Parameter
at Infinite Dilution
(1)
Polymer |
Solvent |
χ∞ |
Polystyrene |
Cyclohexane |
0.510 |
Poly(dimethyl siloxane) |
2-butanone |
0.500 |
Poly(methacrylamide) |
Water |
0.500 |
Polypropylene |
Benzene |
0.498 |
Polyacrylamide |
Water |
0.495 |
Polyisobutylene |
2-Butanone |
0.495 |
Poly(methyl methacrylate) |
Tetrahydrofuran |
0.494 |
Poly(vinyl alcohol) |
Water |
0.494 |
Poly(n-butyl methacrylate) |
Isopropanol |
0.494 |
Poly(n-butyl methacrylate) |
Ethanol |
0.492 |
Poly(o-chlorostyrene) |
Butyl acetate |
0.490 |
Poly(p-chlorostyrene) |
Butyl acetate |
0.490 |
Polystyrene |
2-Butanone |
0.490 |
Hydroxypropyl cellulose |
Water |
0.480 |
Poly(methyl methacrylate) |
Acetone |
0.480 |
Polyisobutylene |
n-Pentane |
0.480 |
Polyisobutylene |
Benzene |
0.479 |
Poly(dimethyl siloxane) |
chlorobenzene |
0.475 |
Poly(p-chlorostyrene) |
Toluene |
0.475 |
Polystyrene |
Benzene |
0.475 |
Poly(o-chlorostyrene) |
Toluene |
0.470 |
Polystyrene |
Ethylbenzene |
0.450 |
Poly(methyl methacrylate) |
Benzene |
0.445 |
Polyisobutylene |
Pentene |
0.445 |
Polystyrene |
Cumene |
0.444 |
Polystyrene |
2-butanone |
0.441 |
Poly(dimethyl siloxane) |
Cyclohexane |
0.440 |
Poly(vinyl acetate) |
2-butanone |
0.430 |
Polyisobutylene |
Cyclohexane |
0.430 |
Poly(vinyl acetate) |
Acetone |
0.425 |
Poly(vinyl acetate) |
Benzene |
0.420 |
Poly(dimethyl siloxane) |
Cyclohexane |
0.409 |
Poly(vinyl chloride |
2-butanone |
0.408 |
Poly(vinyl acetate) |
dimethylphthalate |
0.407 |
Poly(cis-isoprene) |
Benzene |
0.400 |
Poly(cis-isoprene) |
Cyclohexane |
0.310 |