POLYMER CLASS | Polyvinylester |
COMMON NAMES | Poly(vinyl formate) |
STRUCTURE BASED NAME | Poly(formyloxyethylene) |
ACRONYMS | |
CAS # | |
CurlySMILES | C{-}C{n+}OC=O |
CAS # | 692-45-5 |
COMMON NAMES | Vinyl formate |
SMILES | C=COC=O |
Std. InChI | 1S/C3H4O2/c1-2-5-3-4/h2-3H,1H2 |
Std. InChIKey | GFJVXXWOPWLRNU-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | > 53.4 | |
Density ρ | g mL-1 | < 1.35 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 304 - 315 | 307 |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none | 1.47 - 1.48 | 1.48 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 72.06 | |
Van-der-Waals Volume VvW | mL mol-1 | 32.01 | |
Molar Volume Vm | mL mol-1 | 52.7 - 58.4 | 55.5 |
Density ρ | g mL-1 | 1.23 - 1.37 | 1.30 |
Solubility Parameter δ | MPa1/2 | 17.8 - 18.7 | 18.3 |
Molar Cohesive Energy Ecoh | J mol-1 | 17500 - 18500 | 18000 |
Glass Transition Temperature Tg | K | 285 - 301 | 293 |
Molar Heat Capacity Cp | J (mol K)-1 | 76
- 92 116 - 122 | 85 (s) 118 (l,r) |
Entanglement Molecular Weight Me | g mol-1 | 4100 - 4800 | 4450 |
Index of Refraction n | none | 1.42 - 1.48 | 1.44 |