Poly(vinyl ethyl ketone)
CROW logo
Poly(vinyl ethyl ketone)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyvinylketone
COMMON NAMESPoly(vinyl ethyl ketone)
STRUCTURE BASED NAME Poly(ethoylethylene)
ACRONYMS
CAS # 25104-37-4
CurlySMILES C{-}(C(=O)CC)C{n+}
 

IDENTIFIERS OF MONOMER(S)

CAS # 1629-58-9
COMMON NAMESVinyl ethyl ketone
SMILES CCC(=O)C=C
Std. InChI 1S/C5H8O/c1-3-5(6)4-2/h3H,1,4H2,2H3
Std. InChIKey JLIDVCMBCGBIEY-UHFFFAOYSA-N
STRUCTURE
Vinyl ethyl ketone
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-181.6 - 82.081.8
Density ρg mL-1 1.031.03
Solubility Parameter δMPa1/2 19.0 - 22.120.2
Molar Cohesive Energy EcohJ mol-1 29500 - 4000033500
Glass Transition Temperature TgK > 213
Molar Heat Capacity CpJ (mol K)-1
Entanglement Molecular Weight Meg mol-1
Index of Refraction nnone
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 84.12
Van-der-Waals Volume VvWmL mol-1 52.34
Molar Volume VmmL mol-178.8 - 79.579.3
Density ρg mL-1 1.06 - 1.071.06
Solubility Parameter δMPa1/2 19.6 - 22.020.6
Molar Cohesive Energy EcohJ mol-1 30400 - 3850033500
Glass Transition Temperature TgK 268
Molar Heat Capacity CpJ (mol K)-1171 - 175173
Entanglement Molecular Weight Meg mol-16800 - 102008500
Index of Refraction nnone1.47 - 1.501.49
back to top