Poly(vinyl chloride)
CROW logo
Poly(vinyl chloride)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyhaloolefins
COMMON NAMESPoly(vinyl chloride), Tygon®, Vestolit®, Solvic®, Geon™, Plioflex®, Pevikon™, OxyVinyls®, Formolon®, Benvic®
STRUCTURE BASED NAME Poly(chloroethylene)
ACRONYMS PVC
CAS # 9002-86-2
CurlySMILES C{-}(Cl)C{n+}
 

IDENTIFIERS OF MONOMER(S)

CAS # 75-01-4
COMMON NAMESChloroethene
SMILES ClC=C
Std. InChI 1S/C2H3Cl/c1-2-3/h2H,1H2
Std. InChIKey BZHJMEDXRYGGRV-UHFFFAOYSA-N
STRUCTURE
Chloroethen
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-145.1 - 45.245.2
Density ρg mL-1 1.38 - 1.391.38
Solubility Parameter δMPa1/2 18.2 - 22.119.6
Molar Cohesive Energy EcohJ mol-1 15000 - 2200017300
Glass Transition Temperature TgK 344 - 354
370 - 380
350
375
Molar Heat Capacity CpJ (mol K)-158 - 6862
Entanglement Molecular Weight Meg mol-15400
Index of Refraction nnone1.51 - 1.551.53
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 62.50
Van-der-Waals Volume VvWmL mol-1 28.82
Molar Volume VmmL mol-144.6 - 45.845.3
Density ρg mL-1 1.37 - 1.401.38
Solubility Parameter δMPa1/2 18.5 - 19.419.1
Molar Cohesive Energy EcohJ mol-1 15600 - 1710016600
Glass Transition Temperature TgK 345 - 354350
Molar Heat Capacity CpJ (mol K)-165 - 6866
Entanglement Molecular Weight Meg mol-13750 - 81505750
Index of Refraction nnone1.52 - 1.541.53

  Last updated: January 8, 2016

back to top