POLYMER CLASS | Polyacrylates |
COMMON NAMES | Poly(sec-butyl acrylate) |
STRUCTURE BASED NAME | Poly(sec-butyl propenoate) |
ACRONYMS | |
CAS # | |
CurlySMILES | C{-}C{n+}(C(=O)OC(C)CC) |
CAS # | 2998-08-5 |
COMMON NAMES | sec-Butyl acrylate |
SMILES | CC(OC(=O)C=C)CC |
Std. InChI | 1S/C7H12O2/c1-4-6(3)9-7(8)5-2/h5-6H,2,4H2,1,3H3 |
Std. InChIKey | RNOOHTVUSNIPCJ-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 122.1 | |
Density ρ | g mL-1 | > 1.05 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 250 - 256 | 253 |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 128.17 | |
Van-der-Waals Volume VvW | mL mol-1 | 76.76 | |
Molar Volume Vm | mL mol-1 | 117.0 - 123.0 | 119.3 |
Density ρ | g mL-1 | 1.04 - 1.10 | 1.07 |
Solubility Parameter δ | MPa1/2 | 17.6 - 18.5 | 18.0 |
Molar Cohesive Energy Ecoh | J mol-1 | 37400 - 40000 | 38600 |
Glass Transition Temperature Tg | K | 231 - 275 | 250 |
Molar Heat Capacity Cp | J (mol K)-1 | 241 - 248 | 243 |
Entanglement Molecular Weight Me | g mol-1 | 16700 - 17900 | 17300 |
Index of Refraction n | none | 1.47 - 1.48 | 1.47 |