POLYMER CLASS | Polyvinylether |
COMMON NAMES | Poly(propyl vinyl ether), Poly(vinyl propyl ether) |
STRUCTURE BASED NAME | Poly(propoxyethylene) |
ACRONYMS | |
CAS # | |
CurlySMILES | C{-}C{n+}(OCCC) |
CAS # | 764-47-6 |
COMMON NAMES | Propyl vinyl ether |
SMILES | CCCOC=C |
Std. InChI | 1S/C5H10O/c1-3-5-6-4-2/h4H,2-3,5H2,1H3 |
Std. InChIKey | OVGRCEFMXPHEBL-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 85.8 - 91.6 | 87.8 |
Density ρ | g mL-1 | 0.94 - 1.00 | 0.94 |
Solubility Parameter δ | MPa1/2 | 16.9 - 19.3 | 18.1 |
Molar Cohesive Energy Ecoh | J mol-1 | 26200 - 34100 | 28600 |
Glass Transition Temperature Tg | K | 224 | |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 86.13 | |
Van-der-Waals Volume VvW | mL mol-1 | 53.37 | |
Molar Volume Vm | mL mol-1 | 90.7 - 92.5 | 91.6 |
Density ρ | g mL-1 | 0.93 - 0.95 | 0.94 |
Solubility Parameter δ | MPa1/2 | 16.8 - 18.1 | 17.3 |
Molar Cohesive Energy Ecoh | J mol-1 | 26200 - 27500 | 27300 |
Glass Transition Temperature Tg | K | 218 - 223 | 222 |
Molar Heat Capacity Cp | J (mol K)-1 | 176 - 185 | 181 |
Entanglement Molecular Weight Me | g mol-1 | 8500 - 10200 | 9300 |
Index of Refraction n | none | 1.45 - 1.47 | 1.46 |