Poly(p-phenylene)
CROW logo
Poly(p-phenylene)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyphenylenes
COMMON NAMESPoly(p-phenylene)
STRUCTURE BASED NAME Poly(1,4-phenylene)
ACRONYMS PPP
CAS #
CurlySMILES c1{-}cc{n+}(ccc1)
 

IDENTIFIERS OF MONOMER(S)

CAS # 1535-73-5
COMMON NAMES 1,4-Dibromobenzene
SMILES Brc1ccc(cc1)Br
Std. InChI InChI=1S/C6H4Br2/c7-5-1-2-6(8)4-3-5/h1-4H
Std. InChIKey SWJPEBQEEAHIGZ-UHFFFAOYSA-N
STRUCTURE
p-dibromobenzene
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-1 67.3 - 69.868.6
Density ρg mL-1 1.09 -1.131.11
Solubility Parameter δMPa1/2
Molar Cohesive Energy EcohJ mol-1
Glass Transition Temperature TgK > 538 
Molar Heat Capacity CpJ (mol K)-1 84.5
Entanglement Molecular Weight Meg mol-1
Index of Refraction nnone   
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 76.1
Van-der-Waals Volume VvWmL mol-1 45.6
Molar Volume VmmL mol-1 65.5 - 70.568.2
Density ρg mL-1 1.08 - 1.161.12
Solubility Parameter δMPa1/2 19.6 - 20.320.2
Molar Cohesive Energy EcohJ mol-1 27000 - 2800027800
Glass Transition Temperature TgK 539 - 581558
Molar Heat Capacity CpJ (mol K)-1 78.7 - 87.082.9
Entanglement Molecular Weight Meg mol-1 4100 - 105006000
Index of Refraction nnone 1.61 - 1.701.65

  Last updated: September 23, 2015

back to top