POLYMER CLASS | Polyacrylates |
COMMON NAMES | Poly(n-octyl acrylate) |
STRUCTURE BASED NAME | Poly(n-octyl propenoate) |
ACRONYMS | |
CAS # | 25266-13-1 |
CurlySMILES | C{-}C{n+}(C(=O)OCCCCCCCC) |
CAS # | 2499-59-4 |
COMMON NAMES | n-Octyl acrylate |
SMILES | CCCCCCCCOC(=O)C=C |
Std. InChI | InChI=1S/C11H20O2/c1-3-5-6-7-8-9-10-13-11(12)4-2/h4H,2-3,5-10H2,1H3 |
Std. InChIKey | ANISOHQJBAQUQP-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 188 | |
Density ρ | g mL-1 | 0.98 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 208 | |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | 15200 | |
Index of Refraction n | none | 1.46 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 184.3 | |
Van-der-Waals Volume VvW | mL mol-1 | 117.9 | |
Molar Volume Vm | mL mol-1 | 179 - 187 | 183 |
Density ρ | g mL-1 | 0.99 - 1.03 | 1.01 |
Solubility Parameter δ | MPa1/2 | 17.5 - 18.4 | 17.9 |
Molar Cohesive Energy Ecoh | J mol-1 | 55900 - 60700 | 58400 |
Glass Transition Temperature Tg | K | 205 - 229 | 216 |
Molar Heat Capacity Cp | J (mol K)-1 | 359 - 376 | 366.5 |
Entanglement Molecular Weight Me | g mol-1 | 38900 - 39900 | 39400 |
Index of Refraction n | none | 1.46 - 1.49 | 1.47 |
Last updated: November 18, 2015