POLYMER CLASS | Polymethacrylate |
COMMON NAMES | Poly(cyclohexyl methacrylate) |
STRUCTURE BASED NAME | Poly(cyclohexyl 2-methylpropenoate) |
ACRONYMS | |
CAS # | 25768-50-7 |
CurlySMILES | C{-}C{n+}(C)(C(=O)OC1CCCCC1) |
CAS # | 101-43-9 |
COMMON NAMES | Cyclohexyl methacrylate |
SMILES | O=C(C(=C)C)OC1CCCCC1 |
Std. InChI | 1S/C10H16O2/c1-8(2)10(11)12-9-6-4-3-5-7-9/h9H,1,3-7H2,2H3 |
Std. InChIKey | OIWOHHBRDFKZNC-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 152.7 - 153.2 | 153 |
Density ρ | g mL-1 | 1.10 | 1.10 |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 324 - 406 | 380 (343) |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | 34000 - 35500 | 34500 |
Index of Refraction n | none | 1.51 | 1.51 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 168.24 | |
Van-der-Waals Volume VvW | mL mol-1 | 100.33 | |
Molar Volume Vm | mL mol-1 | 151.1 - 151.9 | 151.6 |
Density ρ | g mL-1 | 1.11 | 1.11 |
Solubility Parameter δ | MPa1/2 | 18.3 - 18.6 | 18.5 |
Molar Cohesive Energy Ecoh | J mol-1 | 50900 - 52600 | 51900 |
Glass Transition Temperature Tg | K | 367 - 373 | 370 |
Molar Heat Capacity Cp | J (mol K)-1 | 212 - 258 | 229 |
Entanglement Molecular Weight Me | g mol-1 | 21500 - 31500 | 26500 |
Index of Refraction n | none | 1.51 | 1.51 |
Last updated: Febr. 25, 2020