Cpoly(bisphenol F carbonate)
CROW logo
Poly(bisphenol F carbonate)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polycarbonates
COMMON NAMESPoly(bisphenol F carbonate), Poly[methane bis(4-phenyl)carbonate]
STRUCTURE BASED NAME Poly(oxycarbonyloxy-1,4-phenylenemethylene-1,4-phenylene)
ACRONYMS
CAS #
CurlySMILES C{-}(=O)Oc1ccc(cc1)Cc2ccc(cc2)O{n+}
 

IDENTIFIERS OF MONOMER(S)

CAS # 620-92-8.75-44-5
COMMON NAMESBisphenol F + Phosgene
SMILES Oc1ccc(cc1)Cc1ccc(cc1)O.ClC(=O)Cl
Std. InChI 1S/C13H12O2/c14-12-5-1-10(2-6-12)9-11-3-7-13(15)8-4-11/h1-8,14-15H,9H2.1S/CCl2O/c2-1(3)4
Std. InChIKey PXKLMJQFEQBVLD-UHFFFAOYSA-N.YGYAWVDWMABLBF-UHFFFAOYSA-N
STRUCTURE
Poly(bisphenol F carbonate)
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-1182.4
Density ρg mL-1 1.24
Solubility Parameter δMPa1/2
Molar Cohesive Energy EcohJ mol-1
Glass Transition Temperature TgK 393 - 420407
Molar Heat Capacity CpJ (mol K)-1
Entanglement Molecular Weight Meg mol-1
Index of Refraction nnone
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 226.23
Van-der-Waals Volume VvWmL mol-1 120.37
Molar Volume VmmL mol-1176.5 - 179.1177.8
Density ρg mL-1 1.26 - 1.281.27
Solubility Parameter δMPa1/2 21.4 - 21.721.6
Molar Cohesive Energy EcohJ mol-1 81300 - 8470082600
Glass Transition Temperature TgK 405 - 449427
Molar Heat Capacity CpJ (mol K)-1249 - 269259
Entanglement Molecular Weight Meg mol-12350 - 24502350
Index of Refraction nnone1.59 - 1.641.62
back to top