POLYMER CLASS | Polycarbonates |
COMMON NAMES | Poly(bisphenol B carbonate) |
STRUCTURE BASED NAME | Poly[oxycarbonyloxy-1,4-phenylene(ethylmethylmethylene)-1,4-phenylene] |
ACRONYMS | |
CAS # | |
CurlySMILES | C{-}(=O)Oc1ccc(cc1)C(CC)(C)c2ccc(cc2)O{n+} |
CAS # | 77-40-7.75-44-5 |
COMMON NAMES | Bisphenol B + Phosgene |
SMILES | CCC(c1ccc(cc1)O)(c1ccc(cc1)O)C.ClC(=O)Cl |
Std. InChI | 1S/C16H18O2/c1-3-16(2,12-4-8-14(17)9-5-12)13-6-10-15(18)11-7-13/h4-11,17-18H,3H2,1-2H3.1S/CCl2O/c2-1(3)4 |
Std. InChIKey | HTVITOHKHWFJKO-UHFFFAOYSA-N.YGYAWVDWMABLBF-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 227.4 | |
Density ρ | g mL-1 | 1.18 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 407 - 422 | 415 |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none | 1.58 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 268.31 | |
Van-der-Waals Volume VvW | mL mol-1 | 151.20 | |
Molar Volume Vm | mL mol-1 | 225.7 - 226.6 | 226.2 |
Density ρ | g mL-1 | 1.18 - 1.19 | 1.19 |
Solubility Parameter δ | MPa1/2 | 20.0 - 20.2 | 20.1 |
Molar Cohesive Energy Ecoh | J mol-1 | 90800 - 92400 | 91400 |
Glass Transition Temperature Tg | K | 398 - 430 | 414 |
Molar Heat Capacity Cp | J (mol K)-1 | 321 - 337 | 330 |
Entanglement Molecular Weight Me | g mol-1 | 2700 - 2800 | 2750 |
Index of Refraction n | none | 1.57 - 1.61 | 1.59 |