POLYMER CLASS | Polyhalostyrene |
COMMON NAMES | Poly(3-chlorostyrene) |
STRUCTURE BASED NAME | Poly[1-(3-chlorophenyl)ethane-1,2-diyl], Poly(3-chlorophenylethylene) |
ACRONYMS | |
CAS # | 9022-52-0 |
CurlySMILES | C{-}C{n+}(c1cc(Cl)ccc1) |
CAS # | |
COMMON NAMES | 3-Chlorostyrene |
SMILES | C=Cc1cccc(c1)Cl |
Std. InChI | 1S/C8H7Cl/c1-2-7-4-3-5-8(9)6-7/h2-6H,1H2 |
Std. InChIKey | BOVQCIDBZXNFEJ-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 114 | |
Density ρ | g mL-1 | 1.22 | |
Solubility Parameter δ | MPa1/2 | 19.3 | |
Molar Cohesive Energy Ecoh | J mol-1 | 42300 | |
Glass Transition Temperature Tg | K | 363 | |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 138.59 | |
Van-der-Waals Volume VvW | mL mol-1 | 74.08 | |
Molar Volume Vm | mL mol-1 | 111 - 116 | 113.5 |
Density ρ | g mL-1 | 1.19 - 1.25 | 1.22 |
Solubility Parameter δ | MPa1/2 | 19.1 - 20.0 | 19.6 |
Molar Cohesive Energy Ecoh | J mol-1 | 42400 - 44400 | 43500 |
Glass Transition Temperature Tg | K | 391 - 410 | 399 |
Molar Heat Capacity Cp | J (mol K)-1 | 141 - 152 | 147 |
Entanglement Molecular Weight Me | g mol-1 | 22000 - 42000 | 32000 |
Index of Refraction n | none | 1.59 - 1.60 | 1.60 |