POLYMER CLASS | Polyphenylethers |
COMMON NAMES | Poly(2,6-diphenyl-p-phenylene oxide), Poly(2,6-diphenylphenol) |
STRUCTURE BASED NAME | Poly(oxy-2,6-diphenyl-p-phenylene) |
ACRONYMS | |
CAS # | |
CurlySMILES | O{-}c1c(c2ccccc2)cc(n+}(cc1(c3ccccc3)) |
CAS # | 2432-11-3 |
COMMON NAMES | 2,6-Diphenylphenol |
SMILES | Oc1c(cccc1c1ccccc1)c1ccccc1 |
Std. InChI | 1S/C18H14O/c19-18-16(14-8-3-1-4-9-14)12-7-13-17(18)15-10-5-2-6-11-15/h1-13,19H |
Std. InChIKey | ATGFTMUSEPZNJD-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 214.3 | |
Density ρ | g mL-1 | 1.14 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 493 - 500 | 497 |
Molar Heat Capacity Cp | J (mol K)-1 | 273 | |
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none | 1.60 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 244.29 | |
Van-der-Waals Volume VvW | mL mol-1 | 138.70 | |
Molar Volume Vm | mL mol-1 | 206.5 - 217.6 | 212.0 |
Density ρ | g mL-1 | 1.12 - 1.18 | 1.15 |
Solubility Parameter δ | MPa1/2 | 20.0 - 21.2 | 20.6 |
Molar Cohesive Energy Ecoh | J mol-1 | 87400 - 93200 | 89600 |
Glass Transition Temperature Tg | K | 489 - 500 | 495 |
Molar Heat Capacity Cp | J (mol K)-1 | 253 - 271 | 261 |
Entanglement Molecular Weight Me | g mol-1 | 9150 - 14500 | 12000 |
Index of Refraction n | none | 1.61 - 1.67 | 1.63 |