POLYMER CLASS | Polymethacrylate |
COMMON NAMES | Poly(2-chloroethyl methacrylate) |
STRUCTURE BASED NAME | Poly(2-chloroethyl 2-methylpropenoate) |
ACRONYMS | |
CAS # | |
CurlySMILES | C{-}C{n+}(C)(C(=O)OCCCl) |
CAS # | 1888-94-4 |
COMMON NAMES | 2-Chloroethyl methacrylate |
SMILES | CC(=C)C(=O)OCCCl |
Std. InChI | 1S/C6H9ClO2/c1-5(2)6(8)9-4-3-7/h1,3-4H2,2H3 |
Std. InChIKey | GPOGMJLHWQHEGF-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 112.6 | |
Density ρ | g mL-1 | 1.32 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 365 | |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | 24600 | |
Index of Refraction n | none | 1.49 - 1.52 | 1.50 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 148.6 | |
Van-der-Waals Volume VvW | mL mol-1 | 74.7 | |
Molar Volume Vm | mL mol-1 | 112.4 - 115.0 | 113.7 |
Density ρ | g mL-1 | 1.29 - 1.32 | 1.31 |
Solubility Parameter δ | MPa1/2 | 19.1 - 19.8 | 19.6 |
Molar Cohesive Energy Ecoh | J mol-1 | 40900 - 44600 | 43600 |
Glass Transition Temperature Tg | K | 342 - 369 | 355 |
Molar Heat Capacity Cp | J (mol K)-1 | 181 - 191 | 187 |
Entanglement Molecular Weight Me | g mol-1 | 23400 - 35500 | 29500 |
Index of Refraction n | none | 1.51 - 1.52 | 1.52 |