Poly(1,4-phenylene sulfide)
CROW logo
Poly(1,4-phenylene sulfide)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polythioethers
COMMON NAMESPoly(1,4-phenylene sulfide), Ryton ®, Fortron®, Tedur®, Supec®
STRUCTURE BASED NAME Poly(thio-1,4-phenylene)
ACRONYMS PPS
CAS # 25212-74-2
CurlySMILES S{-}c1ccc{-}(cc1)
 

IDENTIFIERS OF MONOMER(S)

CAS # 1313-82-2.106-46-7
COMMON NAMES1,4-Dichlorobenzene + Disodium sulfide
SMILES Clc1ccc(cc1)Cl.[Na]S[Na]
Std. InChI 1S/C6H4Cl2/c7-5-1-2-6(8)4-3-5/h1-4H.1S/2Na.S
Std. InChIKey OCJBOOLMMGQPQU-UHFFFAOYSA-N.CXPWOVUZRAFMDA-UHFFFAOYSA-N
STRUCTURE
Poly(1,4-phenylenesulfide)
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-1 80.7 - 81.980.1
Density ρg mL-1 1.32 - 1.341.33
Solubility Parameter δMPa1/2
Molar Cohesive Energy EcohJ mol-1
Glass Transition Temperature TgK 353 - 383363
Molar Heat Capacity CpJ (mol K)-1110
Entanglement Molecular Weight Meg mol-1
Index of Refraction nnone
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 108.16
Van-der-Waals Volume VvWmL mol-1 55.5
Molar Volume VmmL mol-183.3 - 86.685.1
Density ρg mL-1 1.25 - 1.301.27
Solubility Parameter δMPa1/2 20.7 - 22.121.1
Molar Cohesive Energy EcohJ mol-1 37000 - 4050038000
Glass Transition Temperature TgK 363 - 369366
Molar Heat Capacity CpJ (mol K)-1103 - 112108
Entanglement Molecular Weight Meg mol-12700 - 42003200
Index of Refraction nnone1.68 - 1.821.71

  Last updated: October 12, 2018