Nylon 6-10
CROW logo
Nylon 6,10 - Poly(hexamethylene sebacamide)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyamide
COMMON NAMESNylon 6-10, Polyamide 6-10,  Poly(hexamethylene sebacamide)
STRUCTURE BASED NAME Poly(iminosebacoyliminohexane-1,6-diyl), Poly(iminohexamethyleneiminosebacoyl)]
ACRONYMS PA6-10
CAS #  
CurlySMILES N{-}C(=O)CCCCCCCCC(=O)NCCCCCC{n+}
 

IDENTIFIERS OF MONOMER(S)

CAS #  
COMMON NAMESSebacic Acid, Hexanediamine
SMILES OC(=O)CCCCCCCCC(=O)O.NCCCCCCN
Std. InChI InChI=1S/C10H18O4/c11-9(12)7-5-3-1-2-4-6-8-10(13)14/h1-8H2,(H,11,12)(H,13,14).InChI=1S/C6H16N2/c7-5-3-1-2-4-6-8/h1-8H2
Std. InChIKey HRNRROMY-UHFFFAOYSA-N.NAQMVNRVTILPCV-UHFFFAOYSA-N
STRUCTURE
Nylon 6-10
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-1 271.5
Density ρg mL-1 1.04
Solubility Parameter δMPa1/2   
Molar Cohesive Energy EcohJ mol-1   
Glass Transition Temperature TgK 310 - 343323
Molar Heat Capacity CpJ (mol K)-1 449.1 - 448.0448.5
Entanglement Molecular Weight Meg mol-1   
Index of Refraction nnone 1.53 - 1.551.54
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 282.4
Van-der-Waals Volume VvWmL mol-1 178.8
Molar Volume VmmL mol-1 274.3 - 279.0276.1
Density ρg mL-1 1.01 - 1.031.02
Solubility Parameter δ MPa1/2 22.0 - 24.123.1
Molar Cohesive Energy EcohJ mol-1 133000 - 160000147000
Glass Transition Temperature TgK 295 - 323321
Molar Heat Capacity CpJ (mol K)-1 427 - 449441
Entanglement Molecular Weight Meg mol-1 1500 - 28002050
Index of Refraction nnone 1.50 - 1.511.51

  Last updated: January 13, 2018

back to top