Nylon 12
CROW logo
Nylon 10 - Poly(ω-decanamide)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyamide
COMMON NAMESNylon 10, Poly(ω-decanamide), Poly(decano-10-lactam)
STRUCTURE BASED NAME Poly(imino-1-oxodecamethylene), Poly[imino(1-oxodecane-1,10-diyl)]
ACRONYMS PA10
CAS #  
CurlySMILES N{-}C(=O)CCCCCCCCC{n+}
 

IDENTIFIERS OF MONOMER(S)

CAS # 236-033-4
COMMON NAMES10-Aminodecanoic acid
SMILES NCCCCCCCCCC(=O)O
Std. InChI 1S/C10H21NO2/c11-9-7-5-3-1-2-4-6-8-10(12)13/h1-9,11H2,(H,12,13)
Std. InChIKey XAUQWYHSQICPAZ-UHFFFAOYSA-N
STRUCTURE
Nylon 12
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-1 1661 
Density ρg mL-1 1.021 
Solubility Parameter δMPa1/2
Molar Cohesive Energy EcohJ mol-1
Glass Transition Temperature TgK 315 - 316315
Molar Heat Capacity CpJ (mol K)-1
Entanglement Molecular Weight Meg mol-1
Index of Refraction nnone   
 

Thermo-Physical Properties: Calculated Data

  Last updated: August 7, 2016

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 169.27
Van-der-Waals Volume VvWmL mol-1 109.9
Molar Volume VmmL mol-1 168 - 172170
Density ρg mL-1 0.99 - 1.011.00
Solubility Parameter δMPa1/2 21.1 - 22.6219
Molar Cohesive Energy Ecoh J mol-1 75000 - 8730081800
Glass Transition Temperature TgK 309 - 317314
Molar Heat Capacity CpJ (mol K)-1 260.5 - 274.5270
Entanglement Molecular Weight Meg mol-1 2660 - 17152030
Index of Refraction n none 1.50 1.50

1 Interpolated data
  Last updated: August 7, 2016

back to top