POLYMER CLASS | Polyamide |
COMMON NAMES | Nylon 10-10, Polyamide 10-10, Poly(decamethylene sebacamide) |
STRUCTURE BASED NAME | Poly(iminosebacoyliminodecamethylene), Poly(iminodecanedioyliminodecane-1,10-diyl) |
ACRONYMS | PA10-10 |
CAS # | |
CurlySMILES | N{-}C(=O)CCCCCCCCC(=O)NCCCCCCCCCC{n+} |
CAS # | 111-20-6, 211-471-9 |
COMMON NAMES | Sebacic Acid, 1,10-Decanediamine |
SMILES | OC(=O)CCCCCCCCC(=O)O.NCCCCCCCCCCN |
Std. InChI | InChI=1S/C10H18O4/c11-9(12)7-5-3-1-2-4-6-8-10(13)14/h1-8H2,(H,11,12)(H,13,14).InChI=1S/C10H24N2/c11-9-7-5-3-1-2-4-6-8-10-12/h1-12H2 |
Std. InChIKey | CXMXRPHRNRROMY-UHFFFAOYSA-N.YQLZOAVZWJBZSY-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | ≥ 329 | |
Density ρ | g mL-1 | ≤ 1.03 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 315 - 333 | 323 |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 338.54 | |
Van-der-Waals Volume VvW | mL mol-1 | 219.9 | |
Molar Volume Vm | mL mol-1 | 337 - 345 | 341 |
Density ρ | g mL-1 | 0.98 - 1.01 | 0.99 |
Solubility Parameter δ | MPa1/2 | 21.1 - 22.6 | 21.9 |
Molar Cohesive Energy Ecoh | J mol-1 | 150000 - 175000 | 163500 |
Glass Transition Temperature Tg | K | 309 - 317 | 314 |
Molar Heat Capacity Cp | J (mol K)-1 | 521 - 549 | 539 (s) |
Entanglement Molecular Weight Me | g mol-1 | 1400 - 2700 | 1900 |
Index of Refraction n | none | 1.50 - 1.51 | 1.50 |
Last updated: January 13, 2018