Poly(vinyl benzoate)
CROW logo
Poly(vinyl benzoate)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyvinylester
COMMON NAMESPoly(vinylbenzoate)
STRUCTURE BASED NAME Poly(benzoyloxyethylene)
ACRONYMS  
CAS # 24991-32-0
CurlySMILES C{-}C{n+}(OC(=O)c1ccccc1)
 

IDENTIFIERS OF MONOMER(S)

CAS #  
COMMON NAMESVinyl benzoate
SMILES C=COC(=O)c1ccccc1
Std. InChI InChI=1S/C9H8O2/c1-2-11-9(10)8-6-4-3-5-7-8/h2-7H,1H2
Std. InChIKey KOZCZZVUFDCZGG-UHFFFAOYSA-N
STRUCTURE
Vinyl benzoate
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-1 124 
Density ρg mL-1 1.20 
Solubility Parameter δMPa1/2   
Molar Cohesive Energy EcohJ mol-1   
Glass Transition Temperature TgK 341 - 347344
Molar Heat Capacity CpJ (mol K)-1 163.4 - 165.1 164.2
Entanglement Molecular Weight Meg mol-1   
Index of Refraction nnone 1.52 - 1.581.58
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 148.2
Van-der-Waals Volume VvWmL mol-1 81.4
Molar Volume VmmL mol-1 117 - 123120
Density ρg mL-1 1.20 - 1.271.24
Solubility Parameter δMPa1/2 20.4 - 21.220.8
Molar Cohesive Energy EcohJ mol-1 49400 - 5310051600
Glass Transition Temperature TgK 343 - 361352
Molar Heat Capacity CpJ (mol K)-1 171 - 173172
Entanglement Molecular Weight Me g mol-1 5200 - 8300 6300
Index of Refraction nnone 1.58 - 1.591.59

  Last updated: October 14, 2015