POLYMER CLASS | Polyacrylates |
COMMON NAMES | Poly(sec-butyl methacrylate) |
STRUCTURE BASED NAME | Poly(sec-butyl 2-methylpropenoate) |
ACRONYMS | PsBMA |
CAS # | |
CurlySMILES | C{-}C{n+}(C)(C(=O)OC(C)CC) |
CAS # | |
COMMON NAMES | sec-Butyl methacrylate |
SMILES | CCC(OC(=O)C(=C)C)C |
Std. InChI | 1S/C8H14O2/c1-5-7(4)10-8(9)6(2)3/h7H,2,5H2,1,3-4H3 |
Std. InChIKey | VXTQKJXIZHSXBY-UHFFFAOYSA-N |
STRUCTURE |
![]() |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molar Volume Vm | mL mol-1 | 135 | |
Density ρ | g mL-1 | 1.05 | |
Solubility Parameter δ | MPa1/2 | ||
Molar Cohesive Energy Ecoh | J mol-1 | ||
Glass Transition Temperature Tg | K | 333 | |
Molar Heat Capacity Cp | J (mol K)-1 | ||
Entanglement Molecular Weight Me | g mol-1 | ||
Index of Refraction n | none | 1.48 |
PROPERTY | UNIT | VALUE / RANGE | PREFERRED |
Molecular Weight of Repeat unit | g mol-1 | 142.2 | |
Van-der-Waals Volume VvW | mL mol-1 | 87.0 | |
Molar Volume Vm | mL mol-1 | 133 - 138 | 135 |
Density ρ | g mL-1 | 1.03 - 1.07 | 1.06 |
Solubility Parameter δ | MPa1/2 | 17.3 - 17.8 | 17.6 |
Molar Cohesive Energy Ecoh | J mol-1 | 41200 - 41900 | 41700 |
Glass Transition Temperature Tg | K | 321 - 344 | 329 |
Molar Heat Capacity Cp | J (mol K)-1 | 208 - 225 | 215 |
Entanglement Molecular Weight Me | g mol-1 | 21400 | 21400 |
Index of Refraction n | none | 1.47 - 1.48 | 1.48 |