Poly(propylene sebacate)
CROW logo
Poly(1,3-propylene succinate)
 

NAMES AND IDENTIFIERS OF POLYMER

POLYMER CLASS Polyesters
COMMON NAMES Poly(1,3-propylene succinate), Poly(trimethylene succinate)
STRUCTURE BASED NAME Poly(oxypropane-1,3-diyloxybutanedioyl), Poly(oxypropane-1,3-diyloxysuccinyl)
ACRONYMS  
CAS # 28158-21-6
CurlySMILES O{-}CCCOC(=O)CCC{n+}(=O)
 

IDENTIFIERS OF MONOMER(S)

CAS # 203-740-4, 504-63-2
COMMON NAMES Succinic acid, 1,3-Propanediol
SMILES OC(=O)CCC(=O)O.OCCCO
Std. InChI InChI=1S/C4H6O4/c5-3(6)1-2-4(7)8/h1-2H2,(H,5,6)(H,7,8).InChI=1S/C3H8O2/c4-2-1-3-5/h4-5H,1-3H2
Std. InChIKey KDYFGRWQOYBRFD-UHFFFAOYSA-N.YPFDHNVEDLHUCE-UHFFFAOYSA-N
STRUCTURE
polyester
 

Thermo-Physical Properties: Experimental / Literature Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molar Volume VmmL mol-1   
Density ρg mL-1   
Solubility Parameter δMPa1/2   
Molar Cohesive Energy Ecoh J mol-1    
Glass Transition Temperature TgK 232 
Molar Heat Capacity CpJ (mol K)-1 288 
Entanglement Molecular Weight Meg mol-1
Index of Refraction nnone
 

Thermo-Physical Properties: Calculated Data

PROPERTYUNITVALUE / RANGEPREFERRED
Molecular Weight of Repeat unitg mol-1 158.15
Van-der-Waals Volume VvWmL mol-1 81.6
Molar Volume VmmL mol-1 119 - 125122
Density ρg mL-1 1.26 - 1.341.30
Solubility Parameter δMPa1/2 20.0 - 21.420.8
Molar Cohesive Energy EcohJ mol-1 48000 - 57400 52900
Glass Transition Temperature TgK 241- 249245
Molar Heat Capacity CpJ (mol K)-1 285 - 292286 (l)
Entanglement Molecular Weight Meg mol-1   
Index of Refraction nnone 1.48 - 1.501.49

  Last updated: May 10, 2016

back to top