Characteristic Ratio of Some Polymers

Atactic Polymer  C1
Bisphenol A Polysulfone  2.2
Bisphenol-A diglycidyl ether epoxy resin 4.7
PoIy(1,2-butadiene) 7.4
Poly(1,4-butadiene) 5.3
Poly(1-butene), PB-1 5.8
Poly(2,6-dimethyl-p-phenylene oxide), PPO 3.0
Poly(acrylamide) 12.7
Poly(Bisphenol A carbonate) 2.4
Poly(bisphenol A isophthalate) 3.7
Poly(Bisphenol A terephthalate) 2.6
Poly(caprolactam), Nylon 6 6.2
Poly(dodecyl methacrylate) 14.1
Poly(ethyl acrylate), PEA 9.3
Poly(ethyl methacrylate) 8.0
Poly(ethylene glycol), PEG 6.9
Poly(ethylene terephthalate), PET 4.1
Poly(ethylene), PE 6.9
Poly(hexamethylene adipamide), Nylon 6,6 6.5
Poly(hexyl methacrylate) 12.2
Poly(isobutene), PIB 6.7
Poly(methyl acrylate), PMA 8.1
Poly(methyl methacrylate), PMMA 8.1
Poly(octadecyl methacrylate) 20.6
Poly(octyl methacrylate), POMA 12.1
Poly(propylene), PP 6.0
Poly(tetramethyl Bisphenol A carbonate) 3.1
Poly(vinyl acetate) 9.4
Poly(vinyl chloride), PVC 7.6
Poly(α-methylstyrene)  10.1
Polyacetal, POM 7.5
Polystyrene 10.3